Physical Property Alloy Comparison Analysis |
|
Sn63/Pb37
Common Lead Alloy |
Bi58
Sn42/Bi58 |
LF88
Sn87.1/In10.5/Ag2.0/Sb0.4 |
LF965-35
Sn96.5/Ag3.5 |
LF950-50
Sn95/Ag5 |
SnAgCu
Sn/Ag/Cu |
Sn99C
Sn99.3/Cu0.7 |
Sb05
Sn95/Sb5 |
Melting Point ( oC) |
183E |
139E |
188-197 |
221E |
221-245 |
217-221 |
227E |
232-240 |
Hardness, Brinell |
14HB |
22HB |
13HB |
15HB |
13.7HB |
15HB |
9HB |
15HB |
Tensile Strength, psi |
4442 |
5400 |
7610 |
8245 |
4780 |
4312 |
3190 |
5110 |
Density, g/cc |
8.42 |
8.72 |
7.37 |
7.5 |
7.39 |
7.39 |
7.31 |
7.26 |
Coefficient of
Thermal Expansion |
24.7 |
13.8 |
24.5 |
Pure Sn = 23.5 |
Pure Sn = 23.5 |
Pure Sn = 23.5 |
Pure Sn = 23.5 |
20.09 |
Electrical Resistivity,
(mohm - cm) |
14.5 |
34.5 |
16.3 |
12.3 |
13.7 |
13.0 |
10-15 |
14.5 |
Electrical Conductivity,
% IACS |
11.9 |
4.5 |
14 |
14 |
12.6 |
16.6 |
13.0 |
11.9 |
|